Grade 91 steam pipe: what the Larson-Miller constant does to a 600 °C life
A 2025 study measures creep rupture of Grade 91 steel taken out of service and finds the Larson-Miller constant sits between 16 and 21. We recompute what that spread does to an extrapolated service life.
A power station’s hot reheat pipe runs near 600 °C for decades. Nobody can test a pipe for 300 000 hours before deciding whether it is safe for another ten years, so engineers test short at a higher temperature and carry the answer down to the service temperature with a time-temperature parameter. The oldest and most used one is the Larson-Miller parameter, LMP = T (C + log₁₀ t), with temperature T in kelvin, rupture time t in hours and a constant C that is almost always taken as 20. A 2025 paper in Frontiers in Materials took Grade 91 steel out of real steam pipes, crept it to rupture between 600 and 700 °C, and measured what C actually is. This article recomputes the consequences with the larson-Miller creep calculator; for the short-term strength of the same kind of steel see the stress-strain curve analyser, and for cycling loads the fatigue S-N calculator.
The paper in brief
The authors collected ASME Grade 91 piping that had spent up to about 148 000 hours in ultra-supercritical plants, including welded joints that had served around 117 000 hours at 602 °C and 38 MPa. They then ran iso-stress tests: tests at one stress and several temperatures, from 600 to 700 °C, on both base metal and welded joints, at 34 to 80 MPa.
Their central measurement is simple to state. Plot log₁₀ rupture time against 1/T at a fixed stress and the points fall on a straight line, over the whole 600 to 700 °C range and right down to service-level stresses. The slope and intercept of that line give the Larson-Miller parameter and the constant C, and the authors find C between about 16 and 21 for welded joints and 18 to 21 for base metal, against reference values near 23 and 21. C barely moves with stress or with how strong the particular heat of steel is. Because of that, they argue, the usual estimation method is safe enough: across the C values they measured, the estimated life moves by only about 0.75 to 1.45 times, and their method holds while C is within ±3 of the assumed value.
Checked with the tools
Everything below is a recomputation from the values the paper states in its text. There is no new data here, and no measured curve was redrawn.
Step 1: the straight line in 1/T is the Larson-Miller parameter. Writing the parameter the other way round, log₁₀ t = LMP/T − C, shows that a single Larson-Miller parameter at a fixed stress is a straight line of log₁₀ t against 1/T, of slope LMP and intercept −C. So the paper’s main measurement and the Larson-Miller model are the same statement, and C is read off the intercept. Figure 1 draws that line through the paper’s own worked example, a 10 000 h rupture at 650 °C, for three constants: the lines meet at the test temperature and spread apart at 600 °C.
Step 2: the paper’s worked conversion. Feeding the same rupture into the tool’s param and logTime reproduces the three numbers the paper quotes to the nearest ten thousand hours.
| 10 000 h rupture at 650 °C, carried to 600 °C | Paper says | Tool gives |
|---|---|---|
| C = 10 | about 60 000 h | 63 342 h |
| C = 20 | about 240 000 h | 236 774 h |
| C = 30 | about 890 000 h | 885 062 h |
Step 3: where 0.75 and 1.45 come from. The ratio of two carried-over lives has a tidy closed form. From log₁₀ t₂ = (T₁/T₂)(C + log₁₀ t₁) − C, changing C by ΔC multiplies the carried-over life by 10^(ΔC (T₁/T₂ − 1)) — and the rupture time itself cancels out. For 650 °C down to 600 °C, T₁/T₂ − 1 = 0.0573, so one unit of C is worth 14 % of life.
Solving for the reference constant that reproduces both of the paper’s sensitivity figures gives C = 18.18: at C = 21 the tool returns a ratio of 1.45, and at C = 16 0.75, exactly the paper’s pair. In other words, the paper’s 0.75-to-1.45 window is its measured C span of 16 to 21 seen from a mid-range C of about 18, for a test 50 °C above service. Its ±3 tolerance on C is worth 1.49 times upward and 0.67 times downward on the same basis.
That window is modest only because the tests sit close to the service temperature. Figure 2 shows the same ratio for tests further above 600 °C: a 3-unit error in C is worth 1.49 times for a 650 °C test but 2.19 times for a 700 °C test. The cheaper the test programme, the more the constant matters.
Step 4: fitting C instead of assuming it. To show the whole tool rather than one formula, we built a simulated nine-test set (three stresses of 40, 56 and 80 MPa at 625, 650 and 675 °C) from a straight master curve with C = 18.18, chosen so that 40 MPa at 600 °C gives 270 000 h (our assumption, loosely consistent with the paper’s unfailed 117 000 h service joints). Fitted back with the tool’s fitParam and bestC, the data return C = 18.19 and a scatter of 0.0004 in log₁₀ t. Forcing C = 16 or C = 21 instead still fits the data with a scatter below 0.07 — small enough to look fine on a plot — yet the predicted life at 600 °C and 40 MPa moves from 202 000 h to 391 000 h. Tests spread over 50 °C simply do not pin C tightly, which is why measuring it on service-exposed material, as the paper does, is worth the trouble.
How we made the graphs
The charts and every number come from scripts/blog-figures/grade-91-steel-creep-rupture-larson-miller-constant-service-temperature.mjs in fibub’s public code. It calls param, logTime, fitParam, bestC and ruptureTime from src/lib/sci/creep.ts, the maths behind the larson-Miller creep calculator.
From the paper’s text: the 600 to 700 °C test range, the 10 000 h rupture at 650 °C and its three converted lives, the C ranges 16 to 21 and 18 to 21, the ±3 tolerance and the 0.75 to 1.45 life window. Our assumptions: the reference C of 18.18 (solved so that the tool reproduces the paper’s 1.45 and 0.75), the nine simulated tests in step 4 and the straight master curve behind them, and the 270 000 h anchor at 600 °C and 40 MPa. The paper’s measured rupture times are in its figures, so none of its data points are used or redrawn.
How we test the maths
On every change to fibub, tests/sci.mjs runs tests/sci-tools/larson-miller-calculator.mjs, which pins the creep maths against NumPy and SciPy:
- On the page’s 12 made-up ruptures, the quadratic Larson-Miller fit with C = 20 must give 26 056.089, 1235.753 and −1383.708, with a scatter of 0.07676 in log₁₀ t, as NumPy’s
polyfitdoes; the best-fit C must be 19.5028, as SciPy’sminimize_scalarfinds. - The same fit must predict 33 784 h at 650 °C and 120 MPa, and allow 178.05 MPa for 100 000 h at 600 °C, matching SciPy’s
brentq. - All three parameters must invert exactly: carrying a time to a parameter and back must return it to 1 part in 10¹².
- New with this article: a 10 000 h rupture at 650 °C carried to 600 °C must give 63 342, 236 774 and 885 062 h at C = 10, 20 and 30, and the life ratio from C = 18.18 to C = 21 must be 1.450 and to C = 16 must be 0.750.
Check it yourself
On the larson-Miller creep calculator page, in the Creep-rupture data card:
- Set Temperatures in to °C and paste our nine simulated tests, one per line as temperature, stress, hours: 625, 40, 59400; 625, 56, 17400; 625, 80, 4730; 650, 40, 14200; 650, 56, 4300; 650, 80, 1210; 675, 40, 3660; 675, 56, 1140; 675, 80, 333.
- Set Polynomial in log σ to a straight line and Larson-Miller C to 18.18. The master curve reads about 25 871 − 3279 x (x = log₁₀ σ) with a scatter near 0.000, and the best-fit C shown beside it is 18.19.
- In Predict rupture life and allowable stress, type Temperature 600, Stress 40 and Design life 100000. The Larson-Miller life is about 269 850 h.
- Change Larson-Miller C to 16. The life at 600 °C and 40 MPa falls to about 202 400 h: 0.75 times. Change it to 21 and it rises to about 391 300 h: 1.45 times. Those are the paper’s two sensitivity figures, reproduced from its own C range.
- Leave C at 18.18 and change Stress to 60: about 58 860 h, under a tenth of the 40 MPa life. Creep life is far more sensitive to stress than to C.
What researchers can use it for
- Repeat a published extrapolation before trusting it: paste the rupture table, set the paper’s C, and see whether its 100 000 h stress falls out.
- Report how much your answer depends on C: run the fit at C − 3, C and C + 3 and quote the three lives, as this paper effectively does.
- Design a test programme: the life ratio 10^(ΔC (T_test/T_service − 1)) says how far above service you can afford to test for a given uncertainty in C.
- Compare parameters: fit Sherby-Dorn and Manson-Haferd on the same data; if they disagree with Larson-Miller, the extrapolation is not safe.
- Teach the method: a class can see the master curve collapse tests at three temperatures onto one line, then watch it move as C changes.
The fine print
- Every number here is recomputed from values the paper states in its text. Its measured rupture times are only in its figures, so we have not refitted its data.
- The reference C of 18.18 is our solution for the constant that reproduces the paper’s own 1.45 and 0.75 figures; the paper does not state a reference C.
- The nine-test set in step 4 and the master curve behind it are simulated, not Grade 91 data. Real Grade 91 rupture data curve in log stress and scatter far more.
- Grade 91 welds fail in the heat-affected zone, so a weld’s life is not the base metal’s. The paper treats them separately, and so should any extrapolation.
- A time-temperature parameter assumes the damage mechanism does not change between test and service. The paper notes that for the related Grade 92 the creep activation energy differs by more than a factor of two between short and long times, which is exactly the risk.
Sources
- Yaguchi, M., Kanai, M. and Tamura, K. (2025), Temperature dependence of creep rupture life of long-term serviced Grade 91 steel, Frontiers in Materials 12: 1613803, doi:10.3389/fmats.2025.1613803. Licence CC BY, checked on the Frontiers article page, 2026-11-24. Values used here: ASME Grade 91 hot reheat steam piping removed from ultra-supercritical plants, up to about 148 000 h in service; welded joints QA and QB about 117 000 h at 602 °C and 38 MPa, joint S about 118 000 h at 596 °C and 39 MPa; iso-stress tests from 600 to 700 °C; welded joints tested at 34 to 80 MPa, base metal at 40 to 56 MPa; Larson-Miller constant C from about 16 to 21 for welded joints and 18 to 21 for base metal, against reference values near 23 and 21; the method is said to hold while C is within ±3; the worked conversion of a 10 000 h rupture at 650 °C to 600 °C gives about 60 000 h at C = 10, 240 000 h at C = 20 and 890 000 h at C = 30; across the measured C range the estimated life varies by about 0.75 to 1.45 times.
- Larson, F. R. and Miller, J. (1952), Transactions of the ASME 74: 765-775 (the time-temperature parameter); textbook form as in Dieter, Mechanical Metallurgy, chapter 13.
If you are an author or publisher and want a credit or a passage changed or removed, tell us and we will act quickly.