Ni-P plating: when current efficiency collapses, Faraday's law says how thin the film gets
A 2026 study watches nickel-phosphorus current efficiency fall from 55 % to 1 % as acid is added. We turn those efficiencies into thicknesses with fibub's electroplating tool, and find the printed current density off by a thousand.
Electroplating has one law at its heart: the charge you push through the cell decides how much metal lands, and nothing else. Everything that makes plating hard is the gap between that law and reality — the share of the current that goes into hydrogen instead of metal. A 2026 paper in Coatings measures that share directly for nickel-phosphorus baths, and watches it fall from about 55 % to about 1 % as phosphorous acid is added and the bath turns more acidic. Those efficiencies are exactly what the electroplating needs to turn a current into a thickness, so we closed the loop: from their efficiency to their measured film, and back out to the current density the experiment must really have used. Alongside it, the Nernst calculator gives the potentials that decide whether hydrogen or metal wins, and the gas law calculator turns the wasted charge into litres of gas.
The paper in brief
The authors plated five coatings, S1 to S5, from a nickel sulfate-chloride bath with 0, then increasing amounts of phosphorous acid (H₃PO₃) up to 40 g/L, which is both the phosphorus source and the thing that drives the pH down. Each run lasted 30 minutes at 40 °C with stirring, on a 6 cm² window masked out on stainless steel.
The findings: phosphorus goes into the deposit fast, from about 0.2 at.% with no acid to 20 to 24 at.% in every acid-containing bath. The cathodic current efficiency — the fraction of the charge that becomes coating — collapses: about 55 % for the acid-free S1, under 15 % for S2, and 5 % down to 1 % for S3 to S5. S1 came out about 3.6 µm thick; the rest are “ultrathin” films whose thicknesses appear only in a figure. Despite that, the middle bath S2 gave the best tribology, a steady friction coefficient of about 0.30 against 0.80 for the pure-nickel S1, and every coating passed adhesion testing at rating 0.
Checked with the tools
This is a recomputation from numbers in the paper’s text, using the same Faraday’s-law maths the electroplating runs in the browser: nickel with two electrons per atom, molar mass 58.693 g/mol and density 8.908 g/cm³. No fitting and no simulation.
Step 1: the printed current density cannot be right. The paper states a current density of 0.100 A/m². Put that into the tool with 55 % efficiency and 30 minutes, and the answer is 3.4 nanometres — a thousand times thinner than the 3.6 µm actually measured on S1 (Figure 2). Running the calculation backwards, the current density that gives 3.6 µm in 30 minutes at 55 % efficiency is 0.01065 A/cm², which is 1.065 A/dm², 106.5 A/m², or about 9.9 A per square foot. That is a thoroughly ordinary Watts-bath value, and a round 1.00 A/dm² gives 3.38 µm, within 6 % of what was measured. So the experiment almost certainly ran near 1 A/dm² and the printed unit slipped by three decades. Over the 6 cm² window that is a cell current of about 64 mA, and the metal deposited weighs 19.2 mg.
Step 2: the efficiency collapse, in micrometres. Figure 1 takes that current density and sweeps the efficiency. Because Faraday’s law is linear, the paper’s four efficiencies map straight onto four thicknesses for the same half-hour run:
| Sample | Efficiency (paper) | Thickness in 30 min (tool) |
|---|---|---|
| S1 (no H₃PO₃) | about 55 % | 3.60 µm — matches the measured 3.6 µm |
| S2 (5 g/L) | under 15 % | 0.98 µm |
| S3 | about 5 % | 0.33 µm |
| S5 (40 g/L) | about 1 % | 0.065 µm (65 nm) |
That turns “ultrathin” into numbers. It also puts the paper’s best result in perspective: the coating with the useful friction, S2, is roughly one micrometre thick, so its 0.30 friction coefficient is the behaviour of a thin film on steel, not of a bulk Ni-P layer. Anyone hoping to reproduce it needs to know that, and the paper’s own efficiency value is enough to work it out.
Step 3: where the rest of the charge went. The charge that does not plate metal mostly splits water. Treating the whole remainder as hydrogen (our assumption; some of it reduces phosphorous acid to phosphorus, which is the point of the bath), the tool’s gas side gives about 6.9 mL of hydrogen at 40 °C for the S1 run and about 15.2 mL for S5 — more than twice as much gas from the same current, bubbling at the same small cathode. That is a plain mechanistic reason for the paper’s other observations: more bubbles means more local alkalinity, rougher deposits and pitting risk, and it is why high-phosphorus baths are usually run hotter and at higher current density rather than simply more acidic.
Step 4: how much the density assumption matters. A deposit with 22 at.% phosphorus is lighter than nickel. Repeating the S2 case with a density of 7.3 g/cm³ (our assumption, a typical electroless Ni-P value) and nickel’s molar mass gives 1.20 µm instead of 0.98 µm. So the thicknesses above are good to about 20 % for the phosphorus-rich samples, and essentially exact for S1, whose phosphorus content is 0.2 at.%.
| Check | Paper | Tool gives (recomputed) |
|---|---|---|
| Current density | 0.100 A/m² as printed | 106.5 A/m² (1.065 A/dm²) implied by 3.6 µm at 55 % |
| Thickness at the printed density | — | 3.4 nm in 30 min: a factor of 1000 out |
| S1 thickness | about 3.6 µm | 3.60 µm at 55 % and 1.065 A/dm² (the calibration point) |
| S2 thickness | “ultrathin”, figure only | 0.98 µm (1.20 µm with a Ni-P density) |
| S5 thickness | “ultrathin”, figure only | 65 nm |
| Deposited mass, S1 | not stated | 19.2 mg over 6 cm² |
| Hydrogen from the wasted charge | not stated | 6.9 mL (S1) to 15.2 mL (S5) at 40 °C |
How we made the graphs
The charts and every number come from scripts/blog-figures/ni-p-electrodeposition-current-efficiency-faraday-thickness-current-density.mjs in fibub’s public code. It calls rate (plating rate in µm/h from current density and efficiency), mass, thickness, timeFor, moles and gasVolume from src/lib/sci/faraday.ts, the maths behind the electroplating.
Inputs from the paper’s text: the 30-minute plating time, the 6 cm² area, the 40 °C bath, the four current efficiencies and S1’s 3.6 µm thickness. Nickel’s molar mass, density and the Faraday constant are the standard reference values listed in sources:. Three things are our assumptions: that S1’s deposit is close enough to pure nickel to use nickel’s density (its phosphorus content is 0.2 at.%), that all the non-plating charge makes hydrogen, and the 7.3 g/cm³ used for the Ni-P density sensitivity.
How we test the maths
On every change to fibub, tests/sci.mjs and tests/sci-tools/electroplating-calculator.mjs pin this maths against textbook electrochemistry:
- Copper at 2 A/dm² must plate at 26.46 µm/h and nickel at 1 A/dm² at 12.29 µm/h, the rates quoted in plating handbooks.
- Silver must obey the classic silver-coulometer figure: 1 A for one hour deposits 4.0247 g.
- Thickness, time and current must round-trip: the time worked out for 25 µm at 2 A over 100 cm² at 95 % efficiency must give back 2 A and 25 µm when fed the other way.
- One hour at 1 A must make 0.01866 mol of hydrogen, which is 0.4181 L at 0 °C and 1 atm.
- New with this article: 1.065 A/dm² for 30 minutes at 55 % efficiency must give 3.60 µm of nickel and 19.24 mg over 6 cm², the printed 0.100 A/m² must give 3.38 nm over the same run, and 1 % efficiency must give 65 nm.
Check it yourself
On the electroplating:
- Leave the mode on Thickness. In Metal or gas choose Nickel (Ni, n = 2).
- Set Area plated (cm²) to 6, Current (A) to 0.0639, Time (min) to 30 and Current efficiency (%) to 55.
- It reads a thickness of about 3.60 µm, a mass of about 19.2 mg and a current density of about 1.07 A/dm² — the paper’s measured film, from the paper’s own efficiency.
- Change Current efficiency (%) to 15, then 5, then 1: the thickness falls to 0.98 µm, 0.33 µm and 0.065 µm. That is the paper’s efficiency collapse in thickness.
- Now set Current (A) to 0.00006 (the printed 0.100 A/m² over 6 cm²) with efficiency back at 55: the thickness drops to about 0.0034 µm, which is 3.4 nm. A unit slip of three decades is easy to see this way.
- Switch Metal or gas to Hydrogen gas, keep Current (A) at 0.0639 and Time (min) at 30, set Current efficiency (%) to 45 (the share that did not plate) and Gas temperature (°C) to 40: about 6.9 mL of hydrogen.
What researchers can use it for
- Sanity-check a plating paper before building on it: a current density, a time and a thickness must agree through Faraday’s law, and unit slips show up at once (electroplating).
- Turn a measured current efficiency into the thickness you will actually get, so a tribology or corrosion result is reported with the film thickness it belongs to.
- Budget the hydrogen a low-efficiency bath will make, for ventilation, for stirring and for embrittlement risk, with the tool’s gas side and the gas law calculator.
- Set the plating time for a target thickness on a new bath: measure the efficiency once, then read the time off the tool instead of guessing.
- Check whether metal or hydrogen should win at your pH and potential with the Nernst calculator, before blaming the additives.
The fine print
- The 1.065 A/dm² is our inference from the paper’s own thickness and efficiency, not a value the paper states. If the real efficiency was not 55 %, the inferred density moves in proportion.
- Thicknesses for S2 to S5 assume nickel’s density and molar mass. A real Ni-P deposit at 22 at.% P is less dense, which makes the film thicker for the same charge, by about 20 % at the density we assumed.
- Faraday’s law is exact for the charge that plates; everything uncertain here sits in the current efficiency, which the paper measured and we took as given.
- Phosphorus reduction consumes some of the “wasted” charge, so our hydrogen volumes are upper limits.
- The paper’s tribology, roughness and wettability results are not checked here; only the charge-to-thickness chain is.
Sources
- Reddah, I., Ghelani, L., Santo, D., Neiva, J., Figueiredo, L., Cavaleiro, D., Carvalho, S. and Devesa, S. (2026), Effect of Phosphorous Acid-Induced pH Variation on Ni-P Electrodeposition: Influence on Current Efficiency, Deposition Rate, Surface Properties, and Tribological Performance, Coatings 16(2): 205, doi:10.3390/coatings16020205. Creative Commons Attribution (CC BY) licence, checked on the MDPI article page, 2026-11-24. Values used here: five baths S1 to S5 with 0 to 40 g/L phosphorous acid; plating for 30 min at (40 +/- 1) degrees C with 200 rpm stirring; plated area 6 cm2 masked on a 316L substrate; current density printed as 0.100 A/m2; cathodic current efficiency about 55 % for S1, under 15 % for S2 and about 5 % down to 1 % for S3 to S5; S1 thickness about 3.6 micrometres by profilometry; phosphorus content about 0.2 at.% in S1 and 20 to 24 at.% in S2 to S5; friction coefficient about 0.30 for S2 against about 0.80 for S1; adhesion rating 0 by ISO 2409.
- Faraday constant 96485.33212 C/mol: CODATA recommended values (NIST). Nickel molar mass 58.693 g/mol: IUPAC/CIAAW standard atomic weights. Nickel density 8.908 g/cm3: CRC Handbook of Chemistry and Physics, room temperature.